Table 2: Results of steel tensile data 2.25Cr-1Mo in standardized conditions (SC) and Quenched and Tempered (QT).
Amostra | T (K) | EM (MPa) | YS (MPa) | TSL (MPa) | TE (%) | n |
SC1 | 300 | 210,200 | 442 | 558.2 | 20.2 | 0.14 |
SC2 | 773 | 168,955 | 370 | 490.8 | 26.5 | 0.11 |
SC3 | 873 | 126,500 | 335 | 405.4 | 34.1 | 0.06 |
SC4 | 973 | 73,100 | 180 | 215.1 | 80.1 | 0.04 |
QT1 | 300 | 66,650 | 800 | 1,080.8 | 17.2 | 0.85 |
QT2 | 773 | 53,500 | 780 | 946.5 | 22.5 | 0.64 |
QT3 | 873 | 11,000 | 550 | 606.7 | 30.4 | 0.60 |
QT4 | 973 | 7,850 | 175.9 | 198.7 | 57.3 | 0.41 |